材料说明: This property data is a summary of similar materials in the MatWeb database for the category “Ductile Iron”. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

供应商 点击此处 查看该材料的所有可用供应商。

点击此处 如果您是供应商,并希望了解如何将您的清单添加到本资料中。

 
物理特性公制英语评论
密度 6.647.42 g/cc0.2400.268 磅/英寸Average value: 7.14 g/cc Grade Count:75
 
机械性能公制英语评论
硬度,布氏硬度 120 – 600120 – 600Average value: 240 Grade Count:65
硬度、努氏硬度 162 – 370162 – 370Average value: 219 Grade Count:32
硬度,洛氏硬度 C 11.6 – 55.011.6 – 55.0Average value: 25.4 Grade Count:9
硬度,维氏硬度 151 – 352151 – 352Average value: 206 Grade Count:32
拉伸强度,极限 3451650 兆帕50000240000Average value: 689 MPa Grade Count:77
拉伸强度,屈服 1721450 兆帕24900210000Average value: 501 MPa Grade Count:79
断裂伸长率 0.200 – 40.0 %0.200 – 40.0 %Average value: 9.41 % Grade Count:67
减少面积 2.00 – 10.0 %2.00 – 10.0 %Average value: 5.67 % Grade Count:12
弹性模量 63.0172 GPa914025000 ksiAverage value: 154 GPa Grade Count:34
压缩屈服强度 3312520 兆帕48000365000Average value: 1260 MPa Grade Count:14
泊松比 0.250 – 0.3700.250 – 0.370平均值:0.283 等级计数:23
疲劳强度 207510 兆帕3000074000Average value: 368 MPa Grade Count:15
断裂韧性 44.0110 MPa-m½40.0100 ksi-in½平均值:81.4 MPa-m½ 等级数:7
剪切模量 60.267.6 GPa87309800 ksi平均值:64.5 GPa 等级计数:23
剪切强度 3721480 兆帕54000215000Average value: 865 MPa Grade Count:12
夏比冲击 8.0040.0 J5.9029.5 英尺-磅Average value: 17.3 J Grade Count:11
夏比冲击,无缺口 7.00155 J5.16114 英尺-磅Average value: 83.0 J Grade Count:14
 
电气性能公制英语评论
电阻率 0.000005000.000102 欧姆-厘米0.000005000.000102 欧姆-厘米Average value: 0.0000447 ohm-cm Grade Count:9
磁导率 250 – 750250 – 750Average value: 481 Grade Count:4
 
热性能公制英语评论
线性 CTE 10.618.7 µm/m-°C5.8910.4 µin/in-°FAverage value: 13.5 µm/m-°C Grade Count:16
导热性 13.032.3 W/m-K90.2224 BTU-in/hr-ft²-°FAverage value: 23.7 W/m-K Grade Count:14
熔点 1120 °C2050 °FAverage value: 1120 °C Grade Count:5
最高使用温度,空气 649 °C1200 °FAverage value: 649 °C Grade Count:5
最低使用温度,空气 -30.0 °C-22.0 °FAverage value: -30.0 °C Grade Count:5
 
组件元素属性公制英语评论
铝 0.0500 %0.0500 %Average value: 0.0500 % Grade Count:6
锑,Sb 0.00200 %0.00200 %平均值:0.00200 % 等级计数:6
砷,As 0.0200 %0.0200 %平均值:0.0200 % 等级计数:6
铋 0.00200 %0.00200 %平均值:0.00200 % 等级计数:6
硼,B 0.000600 %0.000600 %平均值:0.000600 % 等级计数:6
镉,Cd 0.00500 %0.00500 %平均值:0.00500 % 等级计数:6
碳,C 2.00 – 4.10 %2.00 – 4.10 %Average value: 3.40 % Grade Count:67
铈 0.00500 – 0.200 %0.00500 – 0.200 %平均值:0.102 % 等级计数:24
铬,Cr 0.0300 – 5.50 %0.0300 – 5.50 %Average value: 0.709 % Grade Count:51
铜,Cu 0.0200 – 1.00 %0.0200 – 1.00 %Average value: 0.595 % Grade Count:44
铁,Fe 53.0 – 96.2 %53.0 – 96.2 %Average value: 87.0 % Grade Count:75
铅,Pb 0.00200 – 0.00300 %0.00200 – 0.00300 %平均值:0.00214 % 等级计数:7
镁 0.0200 – 0.0700 %0.0200 – 0.0700 %Average value: 0.0434 % Grade Count:31
锰,Mn 0.100 – 4.50 %0.100 – 4.50 %Average value: 0.674 % Grade Count:63
钼 0.000 – 2.50 %0.000 – 2.50 %Average value: 0.336 % Grade Count:47
镍 0.0500 – 36.0 %0.0500 – 36.0 %Average value: 8.21 % Grade Count:54
氧气,O 0.00500 %0.00500 %平均值:0.00500 % 等级计数:6
磷,P 0.0150 – 0.250 %0.0150 – 0.250 %Average value: 0.0621 % Grade Count:59
硒,Se 0.0300 %0.0300 %平均值:0.0300 % 等级计数:6
硅,Si 1.00 – 6.00 %1.00 – 6.00 %Average value: 2.67 % Grade Count:75
硫,S 0.00200 – 0.120 %0.00200 – 0.120 %Average value: 0.0215 % Grade Count:45
碲,Te 0.0200 %0.0200 %平均值:0.0200 % 等级计数:6
锡 0.0100 – 0.250 %0.0100 – 0.250 %Average value: 0.0405 % Grade Count:11
钛 0.0400 %0.0400 %平均值:0.0400 % 等级计数:6
钒,V 0.100 – 0.900 %0.100 – 0.900 %Average value: 0.214 % Grade Count:7

以上显示的某些数值可能已从其原始单位进行了转换和/或四舍五入,以便
以一致的格式显示信息。需要更精确的科学或工程数据的用户
计算者可以点击属性值查看原始值以及转换为等效单位的原始值。
我们建议您在计算中只使用原始值或原始换算值,以尽量减少四舍五入。
错误。我们还请您参考 MatWeb 的 使用条款 关于这些信息。

点击此处 查看
该数据表的所有属性值都是最初输入 MatWeb 时的值。





发表评论

为我们的商店建立账户 位置、IP 地址和浏览器类型:我们将把这些信息用于估算税款和运费等目的