Manganese, Mn | |
---|---|
Categories: | MetalNonferrous MetalPure Element |
Material Notes: | Hard Gray Metal. It is almost never used unalloyed, but it is a very important alloying component in a wide variety of steel and other alloys. |
Vendors: | Click here to view all available suppliers for this material. Please click here if you are a supplier and would like information on how to add your listing to this material. |
![]() Download to Excel (requires Excel and Windows)
Add to Folder: |
Physical Properties | Metric | English | Comments | ||
---|---|---|---|---|---|
Density | 7.44 g/cc | 0.269 lb/in³ | |||
Chemical Properties | Metric | English | Comments | ||
Atomic Mass | 54.93805 | 54.93805 | 54.938049 – 1995 | ||
Atomic Number | 25 | 25 | |||
Thermal Neutron Cross Section | 12.6 barns/atom | 12.6 barns/atom | |||
X-ray Absorption Edge | 1.896 Å | 1.896 Å | K | ||
16.268 Å | 16.268 Å | LI | |||
18.896 Å | 18.896 Å | LII | |||
19.2484 Å | 19.2484 Å | LIII | |||
Electrode Potential | -1.05 V | -1.05 V | |||
Electronegativity | 1.55 | 1.55 | Pauling | ||
Ionic Radius | 0.460 Å | 0.460 Å | Crystal Ionic Radius for Valence +7 | ||
0.600 Å | 0.600 Å | Crystal Ionic Radius for Valence +4 | |||
0.660 Å | 0.660 Å | Crystal Ionic Radius for Valence +3 | |||
0.800 Å | 0.800 Å | Crystal Ionic Radius for Valence +2 | |||
Electrochemical Equivalent | 0.684 g/A/h | 0.684 g/A/h | trivalent | ||
1.025 g/A/h | 1.025 g/A/h | divalent | |||
Mechanical Properties | Metric | English | Comments | ||
Hardness, Brinell | 460 | 460 | Converted from Vickers for 3000 kg load/10 mm ball Brinell test. | ||
Hardness, Rockwell A | 75 | 75 | Converted from Vickers. | ||
Hardness, Rockwell C | 48 | 48 | Converted from Vickers. | ||
Hardness, Vickers | 500 | 500 | |||
Tensile Strength, Ultimate | 496 MPa | 71900 psi | Gamma Phase | ||
Tensile Strength, Yield | 241 MPa | 35000 psi | Gamma Phase | ||
Modulus of Elasticity | 159 GPa | 23100 ksi | |||
Bulk Modulus | 92.6 GPa | 13400 ksi | |||
Poissons Ratio | 0.35 | 0.35 | |||
Shear Modulus | 76.4 GPa | 11100 ksi | |||
Electrical Properties | Metric | English | Comments | ||
Electrical Resistivity ![]() | 0.00000688 ohm-cm @Temperature -273 °C | 0.00000688 ohm-cm @Temperature -459 °F | |||
0.00001884 ohm-cm @Temperature -263 °C | 0.00001884 ohm-cm @Temperature -441 °F | ||||
0.0000536 ohm-cm @Temperature -253 °C | 0.0000536 ohm-cm @Temperature -423 °F | ||||
0.0001261 ohm-cm @Temperature -223 °C | 0.0001261 ohm-cm @Temperature -369 °F | ||||
0.0001321 ohm-cm @Temperature -173 °C | 0.0001321 ohm-cm @Temperature -279 °F | ||||
0.0001359 ohm-cm @Temperature -123 °C | 0.0001359 ohm-cm @Temperature -189 °F | ||||
0.0001391 ohm-cm @Temperature -73.0 °C | 0.0001391 ohm-cm @Temperature -99.4 °F | ||||
0.0001419 ohm-cm @Temperature -23.0 °C | 0.0001419 ohm-cm @Temperature -9.40 °F | ||||
0.000143 ohm-cm @Temperature 0.000 °C | 0.000143 ohm-cm @Temperature 32.0 °F | ||||
0.000144 ohm-cm @Temperature 20.0 °C | 0.000144 ohm-cm @Temperature 68.0 °F | ||||
0.0001442 ohm-cm @Temperature 27.0 °C | 0.0001442 ohm-cm @Temperature 80.6 °F | ||||
0.0001461 ohm-cm @Temperature 77.0 °C | 0.0001461 ohm-cm @Temperature 171 °F | ||||
0.0001477 ohm-cm @Temperature 127 °C | 0.0001477 ohm-cm @Temperature 261 °F | ||||
0.0001501 ohm-cm @Temperature 227 °C | 0.0001501 ohm-cm @Temperature 441 °F | ||||
0.0001521 ohm-cm @Temperature 327 °C | 0.0001521 ohm-cm @Temperature 621 °F | ||||
0.0001536 ohm-cm @Temperature 427 °C | 0.0001536 ohm-cm @Temperature 801 °F | ||||
Magnetic Susceptibility | 0.0000115 | 0.0000115 | cgs/g | ||
Thermal Properties | Metric | English | Comments | ||
Heat of Fusion | 271 J/g | 117 BTU/lb | |||
Heat of Vaporization | 4091 J/g | 1760 BTU/lb | |||
CTE, linear ![]() | 22.8 µm/m-°C @Temperature 20.0 – 100 °C | 12.7 µin/in-°F @Temperature 68.0 – 212 °F | |||
26.9 µm/m-°C @Temperature 227 °C | 14.9 µin/in-°F @Temperature 441 °F | ||||
45.7 µm/m-°C @Temperature 1087 °C | 25.4 µin/in-°F @Temperature 1989 °F | Beta Phase | |||
Specific Heat Capacity | 0.379 J/g-°C | 0.0906 BTU/lb-°F | Gas | ||
0.448 J/g-°C | 0.107 BTU/lb-°F | ||||
Thermal Conductivity ![]() | 1.64 W/m-K @Temperature -263 °C | 11.4 BTU-in/hr-ft²-°F @Temperature -441 °F | |||
2.42 W/m-K @Temperature -253 °C | 16.8 BTU-in/hr-ft²-°F @Temperature -423 °F | ||||
4.07 W/m-K @Temperature -223 °C | 28.2 BTU-in/hr-ft²-°F @Temperature -369 °F | ||||
5.81 W/m-K @Temperature -173 °C | 40.3 BTU-in/hr-ft²-°F @Temperature -279 °F | ||||
6.65 W/m-K @Temperature -123 °C | 46.2 BTU-in/hr-ft²-°F @Temperature -189 °F | ||||
7.18 W/m-K @Temperature -73.0 °C | 49.8 BTU-in/hr-ft²-°F @Temperature -99.4 °F | ||||
7.54 W/m-K @Temperature -23.0 °C | 52.3 BTU-in/hr-ft²-°F @Temperature -9.40 °F | ||||
7.68 W/m-K @Temperature 0.000 °C | 53.3 BTU-in/hr-ft²-°F @Temperature 32.0 °F | ||||
7.79 W/m-K @Temperature 20.0 °C | 54.1 BTU-in/hr-ft²-°F @Temperature 68.0 °F | ||||
7.82 W/m-K @Temperature 27.0 °C | 54.3 BTU-in/hr-ft²-°F @Temperature 80.6 °F | ||||
Melting Point | 1244 °C | 2271 °F | |||
Boiling Point | 2061 °C | 3742 °F | |||
Heat of Formation | 0.000 kJ/mol | 0.000 kJ/mol | Crystal | ||
280.7 kJ/mol | 280.7 kJ/mol | Gas | |||
Optical Properties | Metric | English | Comments | ||
Emissivity (0-1) | 0.57 | 0.57 | unoxidized, 650 nm, total spectrum | ||
Reflection Coefficient, Visible (0-1) | 0.45 | 0.45 | 400 nm air-exposed | ||
0.55 | 0.55 | 400 nm polished | |||
Component Elements Properties | Metric | English | Comments | ||
Manganese, Mn | 100 % | 100 % | |||
Descriptive Properties | |||||
CAS Number | 7439-96-5 | ||||
Solubility | Soluble in diluted Acids |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb’s terms of use regarding this information.
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb’s terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.